Questions about how individual parts of claim 1 might be changed. A question may describe something different from what the claim language recites, or a version of it; no view is offered on which.
1.1Copper and tin reaction layers
What ifWhat if a thin tin layer between copper surfaces supplies the liquid for bonding and then reacts to form a copper–tin joint?
Claim language“Sn, Zn, and Al”
A tin layer a few micrometres thick melts between copper surfaces at 235–250 °C and wets both interfaces under pressure. An isothermal hold consumes the free tin and forms copper–tin intermetallics that remain solid at 180 °C.
1.1Indium and silver reaction layers
What ifWhat if an indium layer between silver surfaces supplies the bonding liquid and converts to silver–indium intermetallics?
Claim language“Sn, Zn, and Al”
A thin indium coating melts above 157 °C and wets the adjacent silver surfaces. A hold at 180–220 °C with excess silver consumes the free indium and leaves a joint with a higher remelting temperature than the starting indium layer.
1.2Zinc concentrated at bonding faces
What ifWhat if the sheet contains less than 5 wt % zinc overall and concentrates the zinc in thin bonding skins?
Claim language“Zn accounts for 5 wt % or greater”
Two tin–9 wt % zinc skins together make up 40% of the sheet mass, and a zinc-free tin–aluminum core makes up the balance. The skins supply 3.6 wt % zinc overall and melt near 199 °C to wet the mating surfaces while aluminum-rich regions remain solid in the core.
1.2Aluminum concentrated in the core
What ifWhat if the sheet contains less than 3.5 wt % aluminum overall and concentrates the aluminum in a thin internal layer?
Claim language“Al accounts for 3.5 wt % or greater”
A tin–8 wt % aluminum core makes up one-quarter of the sheet mass, giving an overall aluminum content of 2 wt %. Tin–9 wt % zinc skins melt near 199 °C and wet the mating surfaces while aluminum-rich regions in the core remain solid.
1.2Copper foil carries the load
What ifWhat if copper foil supplies most of the preform mass and thin solder coatings supply the bonding liquid?
Claim language“a remainder being Sn”
An 80 μm copper foil carries a 10 μm tin–zinc solder coating on each face. The coatings melt and wet the mating surfaces during reflow, and the copper foil retains its thickness as a solid spacer.
Section 2 · machine-generated
Variations
Further arrangements of the same subject matter, described here as of the publication date at the foot of this page.
Other field of use
Joining copper fins to heat spreaders
A Sn-Zn-Al foil with two endothermic peaks sits between the nickel-plated foot of each copper fin and a nickel-plated copper heat spreader. A slotted fixture holds the fins upright and keeps the feet seated during heating under nitrogen. The assembly reaches a temperature above the first endothermic peak and below the onset of the second endotherm, and the lower-temperature liquid wets the plated surfaces. The assembly cools in the fixture until the liquid solidifies.
Component substitution
Sn-Bi matrix with sn-sb particles
A composite preform replaces the Sn-Zn-Al filler with a continuous Sn-Bi eutectic matrix containing dispersed Sn-Sb particles. Prealloyed powders are blended and roll compacted into a strip below the melting temperature of the matrix. During assembly, the Sn-Bi matrix melts and wets the mating surfaces while the Sn-Sb particles remain solid. The Sn-Bi matrix solidifies around the particles during cooling.
Parameter or scale variation
Patterned foil for narrow bond lands
A 75 µm Sn-Zn-Al foil with two endothermic peaks is punched into 0.8 mm by 2.0 mm rectangular preforms. Each preform is centered on a 1.0 mm by 2.2 mm nickel-plated copper land beneath a matching tab. Two 50 µm ceramic shims beside each land set the final gap as the lower-temperature phase melts. The fixture holds the tabs against the shims through solidification.
Combination with existing systems
Reflow in a vacuum furnace
A Sn-Zn-Al preform with two endothermic peaks sits between solderable metal surfaces in a graphite fixture inside a vacuum reflow furnace. A thermocouple on a reference assembly tracks the temperature near the joint as the furnace heats under nitrogen. Once the lower-temperature phase forms liquid, the furnace applies a brief vacuum dwell to draw gas from the joint while the higher-temperature phase remains solid. The chamber backfills with nitrogen before the fixture cools.
Automated or data-driven variant
Reflow control from calorimetry data
An automated calorimeter measures the first peak temperature and the onset of the second endotherm on a sample from each Sn-Zn-Al foil lot. Control software pairs the measured temperatures with the lot identifier and selects a reflow setpoint above the first peak and below the second onset. The software checks that the available interval covers the measured temperature variation of the heating station. A thermocouple next to the bond line supplies feedback to the heater during the dwell.
Radiographic feedback for vacuum dwell
A microfocus X-ray source and flat-panel detector image cooled Sn-Zn-Al joints as assemblies leave a vacuum reflow line. Image-processing software segments low-density regions within each joint outline and calculates the projected void area as a fraction of joint area. When the median fraction exceeds a preset limit over a fixed group of assemblies, the controller increases the vacuum dwell for the next group within a qualified time range. The controller holds the reflow temperature between the first peak and the onset of the second endotherm.
Specific version of a part
Cast and rolled ternary foil
Tin, zinc, and aluminum are melted together under an inert cover and cast into a thin strip. The strip is rolled to a 100 μm foil and slit into die-attach preforms.
Atomized and consolidated ternary sheet
Inert gas atomizes a tin–zinc–aluminum melt into powder, which is sieved to retain particles smaller than 45 μm. Pressure consolidates the powder into a strip, and rolling sets the final sheet thickness.
Cast sheet with calorimetric sorting
A nominal 84 wt % tin, 10 wt % zinc, and 6 wt % aluminum melt is chill cast and rolled to sheet. First-heating differential scanning calorimetry at 10 °C per minute selects sheets with exactly two endothermic maxima, one from 190 °C to below 230 °C and the other from 240 °C to below 380 °C.
Blended powders with distinct transitions
Equal masses of a tin–9 wt % zinc powder and a tin-based powder containing 11 wt % zinc and 8 wt % aluminum yield 86 wt % tin, 10 wt % zinc, and 4 wt % aluminum overall. Consolidation below 190 °C retains the two alloy populations, and differential scanning calorimetry selects compacts with exactly two endothermic maxima in the specified temperature intervals.
Section 3 · quoted from USPTO records
Other work
Passages reproduced word for word from two earlier-published U.S. patent documents, placed beside the language of claim 1. No characterization is offered. Each passage is marked A or B for the document it comes from; ¶ numbers are the paragraph numbers in the USPTO’s published full text of that document.
1.1A solder material containing Sn, Zn, and Al, as main components
Among lead free tin-based solder alloys, Sn—Ag—Cu alloys, Sn—Zn alloys, Sn—Ag—In alloys, and Sn—Ag—Cu—In alloys have shown promise.
A · US 2017/0373034 A1 · ¶ 3
Patent Document 3 discloses a lead-free soldering alloy consisting of 0.5 to 5 mass % of Ag, 0.5 to 20 mass % of In, 0.1 to 3 mass % of Bi, 3 mass % or less of an additive element, and balance Sn. The additive element is at least one element selected from Sb, Zn, Ni, Ga, Ge and Cu.
B · US 2022/0040802 A1 · ¶ 6
1.2wherein, with respect to a total of 100 wt %, Zn accounts for 5 wt % or greater and less than 20 wt %, and Al accounts for 3.5 wt % or greater and less than 10 wt %, a remainder being Sn, the solder material has two endothermic peaks in differential scanning calorimetry, and a first alloy phase having an endothermic peak in a range of 190 °C or higher and lower than 230 °C and a second alloy phase having an endothermic peak in a range of 240 °C or higher and lower than 380 °C coexist.
As illustrated by the DSC graph, the solidus temperature of the alloy is about 180.87° C. and the liquidus temperature of the alloy is about 202.66° C. Heat flow peaks at a melting temperature of about 195.21° C.
A · US 2017/0373034 A1 · ¶ 25
An empty cell means only that no passage was reproduced there.
Statements in these documents
In view of the foregoing issues, there is a need for a lead-free solder alloy that has a low liquidus temperature and may be used in demanding applications with a compliance that is comparable to that of lead containing solder alloys.
A · US 2017/0373034 A1 · ¶ 6
The solder alloy is particularly useful for but not limited to solder on pad applications in first level interconnect semiconductor device packaging.
A · US 2017/0373034 A1 · ¶ 7
Incidentally, in a step-soldering where the soldering is performed in multiple stages, the soldering is expected to be performed at an intermediate temperature range between the above-mentioned intermediate temperature and low temperature.
B · US 2022/0040802 A1 · ¶ 4
That is, the property that melts at a temperature below the melting point of the low-temperature soldering alloy represented by Sn-58Bi leads to a possibility of being re-melted in the soldering step of the low-temperature soldering alloy.
B · US 2022/0040802 A1 · ¶ 10