1.1Batch loading of blanks
A cutter shears the triaxial braid into blanks sized for individual half shells. A full-length matched die shapes and consolidates each blank, cools it under pressure, and opens for unloading before the next blank enters.
Generated automatically. Not reviewed by a person. Not legal advice or an opinion.
Questions about how individual parts of claim 1 might be changed. A question may describe something different from what the claim language recites, or a version of it; no view is offered on which.
A cutter shears the triaxial braid into blanks sized for individual half shells. A full-length matched die shapes and consolidates each blank, cools it under pressure, and opens for unloading before the next blank enters.
Unidirectional tapes are cut and stacked in a symmetric layup with axial and balanced off-axis plies. Heated matched dies melt the tape matrix, consolidate the ply interfaces, and form the curved half shell.
Infrared emitters heat both faces of the moving braid above the matrix melting temperature. A short insulated transfer passage feeds the hot braid directly into the forming dies, which close before the matrix solidifies.
The line cools the formed shell rapidly between matched tools, limiting crystallization during the forming pass. A curved fixture supports the cooled shell in an oven that holds the matrix above its glass transition and below its melting point for a controlled annealing dwell.
A matched transfer fixture captures each hot shell section as the molding tools release it. Water circulates through channels in both fixture faces, and the fixture holds the cross section until the matrix is rigid enough for unloading.
Further arrangements of the same subject matter, described here as of the publication date at the foot of this page.
Opposing molds heat, shape, crystallize, and cool a triaxial thermoplastic braid into two furlable half shells with longitudinal flanges. A welding mold joins the mating flanges along both edges to form a tube. A compact reel stores the flattened tube, and paired guide rollers feed it upward so the tube recovers its cross section and supports a temperature and humidity sensor.
A pair of heated pinch rollers at each flange replaces the welding mold downstream of the shell cooling zone. Guide shoes align the mating flanges, and hot air directed between them softens the thermoplastic at the joint before the rollers press the faces together. Water-cooled follow-up rollers hold each seam closed as the joint solidifies.
Induction coils replace resistance heaters in the hot forming station and couple to steel face plates mounted on both opposing mold halves. The coils heat the plates, and the plates conduct heat into the impregnated braid while the mold applies forming pressure. Thermocouples embedded just below the mold faces regulate coil power, and thermal breaks isolate the hot station from the downstream crystallization station.
Each opposing mold pair contains four parallel cavities that process four 50 mm wide braid strips on 80 mm center spacing. The cavities form two matching pairs of half shells with a nominal wall thickness of 0.30 mm and 5 mm wide flanges. The strips advance 100 mm per opening cycle, and two downstream welding stations each join one shell pair.
An inline dry-coupled ultrasonic inspection station sits downstream of the flange welder where the seams have solidified. Opposed wheel probes straddle each flange and measure the ultrasonic signal transmitted through the joint. A line encoder links each measurement to a position along the boom, and the controller records segments with transmission below the threshold established on bonded reference samples.
Opposed laser displacement sensors mounted on a common frame measure the cooled shell at the crown and both shoulders. A line encoder associates each thickness reading with the forming cycle that produced it. When the mean thickness drifts from its setpoint, the controller trims the closed gap of the hot forming mold within preset limits while maintaining the programmed temperatures and line cadence.
A common drive shaft actuates matched cam linkages at the mold stations. Each linkage moves both opposing halves toward the fabric during closure and retracts them together during opening.
A hydraulic actuator presses a heated convex insert into a matching concave cavity while the braid matrix is molten. Ground stops set the closed gap, and the insert surfaces define the transverse curvature of the furlable shell.
For a carbon fiber braid with a polyether ether ketone matrix, the heating zone runs near 380 °C, the crystallization mold near 290 °C, and the cooling zone near 100 °C. Line speed and zone length set the time available for matrix melting, crystallization, and cooling under restraint.
A fourth mold aligns the half shells and clamps their overlapping edge flanges around a thin resistive mesh. Current through the mesh melts the thermoplastic at the interfaces, and the mold maintains pressure until the seams solidify.
Passages reproduced word for word from two earlier-published U.S. patent documents, placed beside the language of claim 1. No characterization is offered. Each passage is marked A or B for the document it comes from; ¶ numbers are the paragraph numbers in the USPTO’s published full text of that document.
Referring to FIG. 5, as the triaxially braided fabric is removed from shipping spool 45 and transferred to its intended variable diameter cylindrical composite forming mold 50, the individual and separate axial yarns within triaxial braided fabric 10, are again, individually and separately, maintained under tension by rollers 52 thereby preventing “slack” from occurring in each separate axial yarn 15.A · US 7,770,837 B1 · ¶ 34
A triaxial braided fabric basically comprises a biaxial braided fabric having an additional matrix of parallel yarns extending the longitudinal, or axial, length of the braided fabric and interwoven into the biaxial braided yarns.A · US 7,770,837 B1 · ¶ 5
The heat shrink enclosure and contents are placed in an oven and heated (typically at about 196° C. (385° F.) when FEP is used as the heat shrink and a polyether block amide is used as an outer jacket material) for a suitable period of time to melt the outer jacket material such that it flows between the braid strands and bonds with the roughened outer surface of the inner liner.B · US 9,622,892 B2 · ¶ 49
An empty cell means only that no passage was reproduced there.
Only Document A has a passage for 1.1 1.2. Only Document B has a passage for 1.3.
Sentences reproduced word for word from these documents (and from a third earlier document, Document C) that state a problem, a purpose or benefit, a field of use, or an application or improvement.
Chopped strand, woven, and biaxial braided mats will generally conform to a concave or convex configuration; however, triaxial braided mats formed on a cylindrical braiding spool will not conform to a convex or concave configured mold without characteristic buckling of the axial yarns because the axial yarns are of equal axial lengths.A · US 7,770,837 B1 · ¶ 8
For example, a coiled reinforcement is typically utilized in a sheath to minimize the possibility of the sheath kinking, and/or to minimize ovalization of the sheath lumen during bending of the sheath.B · US 9,622,892 B2 · ¶ 8
On the other hand, a braid is utilized when it is desired to impart stiffness, pushability, or torqueability to the sheath.B · US 9,622,892 B2 · ¶ 8
Braided structures are often preferred over other types of structures, such as woven structures, because tows of material within the structure can be oriented along non-perpendicular directions and the structures can either conform to a surface upon application or be manufactured in to conform to a specific surface.C · US 2016/0090672 A1 · ¶ 3
Related claim parts: 1.3
Document C: US 2016/0090672 A1, published Mar 31, 2016. Cited for this statement only.
patent.fyi, US 2026/0364897 A1, claim 1, first published 2026-11-23T09:08:10-05:00, https://patent.fyi/US20260364897/, SHA-256 8e7d923e6c76be7abf3bd353a6788341489652337c415b1bad494f2acc00e122